Skip to main content
. 2020 Feb 20;40(2):203–210. [Article in Chinese] doi: 10.12122/j.issn.1673-4254.2020.02.11

2.

不同摩尔比例下分子印迹整体柱的回收率

Different molar ratios of T:M:C of UiO-66-NH2@MIPs and the recovery of the columns

Item T:M:C a (molar ratio) UiO-66-NH2 (mg) Temperature b (℃) Time b (h) Recovery (%)
a: T:M:C (T stands for template, M stands for monomer and C stands for cross-linker). b: The temperature and time of in situ polymerization.
1 1:2:20 5 60 4 51.32
2 1:2:40 5 60 4 61.75
3 1:4:20 5 60 4 79.83
4 1:4:40 5 60 4 81.13
5 1:6:20 5 60 4 67.58
6 1:6:30 5 60 4 95.64
7 1:6:40 5 60 4 73.53