Mechanical properties and sensitivity of hydrogen embrittlement after SSRTT for M10B.

Strain Rate Humidity Fracture Strength/MPa Elongation
/%
PSE/GPa•% Sensitivity of HE /% CH/wppm
10−4 s−1 Air
(about 40% RH)
1380 30.3 41.81 0 0.43 ± 0.04
10−4 s−1 60% RH 1330 29.2 38.84 3.6 0.48 ± 0.05
80% RH 1260 22.5 28.35 25.7 0.91 ± 0.14
100% RH 1200 20.87 25.04 31.1 1.35 ± 0.08
10−6 s−1 60% RH 1050 10.1 10.61 67.0 2.13 ± 0.21
80% RH 1030 7.3 7.52 75.9 2.31 ± 0.15
100% RH 1010 6.6 6.67 78.2 2.23 ± 0.27