Table 2.
Thermogravimetric analysis of the geopolymer samples and PP fiber.
| Mix ID | Temperature range (°C)/Mass loss (%) |
|||
|---|---|---|---|---|
| RT-250 | 250–500 | 500–800 | RT-1000 | |
| GM-0.5-0 | 5,06 | 2,13 | 4,1 | 11,71 |
| GM-1-0 | 3,01 | 1,41 | 4,26 | 8,92 |
| GM-1.5-05 | 3,15 | 1,63 | 3,98 | 9,07 |
| GM-0.5-05 | 3,52 | 2,01 | 3,66 | 9,32 |
| GM-1-05 | 3,08 | 2,98 | 3,80 | 10,11 |
| GM-1.5-05 | 4,93 | 1,93 | 3,97 | 11,16 |
| GM-0.5-1 | 3,02 | 2,52 | 3,83 | 9,60 |
| GM-1-1 | 3,14 | 2,49 | 3,63 | 9,52 |
| GM-1.5-1 | 2,984 | 2,69 | 3,58 | 9,53 |
| PPF | 1 (melting 160) | |||
RT: Room Temperature.