Specimen Tg (°C) Tm (°C) ΔH (J/g) X (%)
I II I II I II I II
PE 300 −116 −113 112 112 162 161 55.35 55.08
PE 400 −120 −123 112 112 157 162 53.72 55.42
PE 500 −120 −116 112 112 153 156 52.14 53.33
PLA 300 −116
−31
48
−120
−31
59
117
148
120 7.6
1.23
9.84 1.38 -
PLA 400 −120
−26
48
−118
−30
59
118
148
120 9.28
1.04
9.28 1.17 -
PLA 500 −122
−31
49
−118
−29
59
117
149
120 7.52
1.38
9.81 1.49 -
TPS-C 300 −117
−28
−120
−30
96 122 91 13.4 31.06 4.59
TPS-C 400 −122
−29
−121
−32
92 122 96.5 17.13 32.94 5.85
TPS-C 500 −113
−28
−120
−30
104 122 89.94 17.17 30.70 5.86
TPS-P 300 −114
−30
−112
−28
102 122 114.5 9.99 39.08 3.41
TPS-P 400 −115
−29
−117
−29
104 123 125.8 10.18 42.92 3.47
TPS-P 500 −114
−30
−117
−30
104 121 116.1 10.43 39.63 3.56

where: I, II—first, and second heating cycle, respectively.