Skip to main content
. 2020 Mar 25;12(4):733. doi: 10.3390/polym12040733

Table 4.

Electrical conductivity of ABS-matrix nanocomposites.

Material Process Dimensions
(mm3)
Percolation Threshold
(wt %)
Content
(wt %)
Electrical Conductivity
(S/m)
Ref.
Pure ABS - - - - 10−15 [37]
ABS + GNPs FDM 10 × 10 × 10 15 10−8–10−5 Current work
ABS + GNPs CM 1 45 × 45 × 2 - 6 10−12 [36]
FDM 2 10−13
ABS + CNTs CM 1 - 10−1
FDM 2 10−2
ABS + CNTs FDM 2 50 × 6 × 1.2 1 6 100–101 [18]
ABS + rGO Hot press Ø 5 cm 0.3 1.3 10−4 [38]
2 10−3
3 10−2
ABS + GNPs CM 1 64 × 64 × 1.2 8–12 20 10−2 [39]
ABS + CNTs 2 8 102
ABS + GNPs Hot press 64 × 64 × 1.2 - 8 10−12 [40]

1 Compression molding. 2 Fused Deposition Modeling.