. 2020 Apr 14;12(4):910. doi: 10.3390/polym12040910

Table 4.

Parameters determined on the basis of DSC measurements for fibers taken at 50 and 200 m/min.

Take-up Velocity
[m/min]
Sample Temp. of Recrystall. Mesophase Enthalpy of Recrystall. Mesophase Temp. of Melting Enthalpy of Melting Total Degree of Crystall.
Tmm [°C] ΔHmm [J/g] Tm [°C] ΔHm [J/g] κ DSC [%]
iPP 100% 102.3 19.26 163.8 96.76 46.7
iPP + rGO-CP (0.1 wt.%) 103.4 18.84 164.9 96.61 46.7
50 iPP + rGO-CP (0.5 wt.%) 102.3 12.31 165.2 96.08 46.8
iPP + rGO-CP (1.0 wt.%) 102.4 5.13 166.0 96.14 46.9
iPP 100% 124.2 9.64 162.5 101.77 49.2
iPP + rGO-CP (0.1 wt.%) 123.0 11.11 163.3 100.60 48.7
200 iPP + rGO-CP (0.5 wt.%) 125.5 11.80 163.3 96.08 46.6
iPP + rGO-CP (1.0 wt.%) 126.7 12.49 163.4 94.91 46.3