Skip to main content
. 2020 May 5;5(19):10680–10686. doi: 10.1021/acsomega.9b04102

Table 1. Results of Thermal Gravimetrical Analysis (τ5, τ10, τ40, °C) and Differential Scanning Calorimetry (Tg, °C) obtained for all the studied nanocomposite fibers based on PEI.

  temperature of decomposition, °C
 
fiber τ5 (5% weight loss) τ10 (10% weight loss) τ40 (40% weight loss) Tg, °C
PEI 522 530 590 217
PEI + 0.05% SWCNTs 520 530 630 216
PEI + 0.1% SWCNTs 524 531 617 216
PEI + 0.2% SWCNTs 524 531 627 217
PEI + 0.5% SWCNTs 518 529 604 216
PEI + 0.5% VGCFs 523 531 597 218
PEI + 1% VGCFs 524 529 614 218
PEI + 3% VGCFs 525 531 613 217
PEI + 5% VGCFs 522 533 644 218