Table 1. Electrical Properties of Transistors Based on the C8-BTBT/PMMA Film Deposited by Spin-Coating on Different Polymer Modification Layers at 2000 rpm.
dielectric | Ci (nF/cm2) | Vth (V) | Ion/Ioff | SS (V/decade) | Ntrapmax (cm–2 eV–1) | average mobility (cm2/V·s) |
---|---|---|---|---|---|---|
SiO2 | 11.4 | –47.7 ± 4.5 | 105–106 | 8.2 ± 0.4 | (9.8 ± 0.5) × 1012 | 0.12 ± 0.09 |
PMMA/SiO2 | 10.2 | –42.3 ± 4.2 | 105–106 | 6.3 ± 0.3 | (7.5 ± 0.3) × 1012 | 0.65 ± 0.25 |
PS/SiO2 | 11.3 | –33.5 ± 3.9 | >107 | 4.7 ± 0.3 | (5.6 ± 0.3) × 1012 | 1.86 ± 1.02 |