Skip to main content
. Author manuscript; available in PMC: 2021 Jul 15.
Published in final edited form as: Int J Biol Macromol. 2020 Mar 28;155:581–587. doi: 10.1016/j.ijbiomac.2020.03.218

Table 1.

Thickness, density, water solubility and moisture content of anchote starch films made from different kind and concentration of plasticizers

Films Thickness (mm) Density (g/cm3) Water Solubility (%) Moisture Content (%)

E30 0.17 ± 0.01a A 1.21 ± 0.04c D 26.70 ± 1.25f B 8.66 ± 0.25d C
E40 0.19 ± 0.04a A 1.20 ± 0.05c D 32.85 ± 1.23e B 7.40 ± 0.55d F
G30 0.18 ± 0.00b A 1.07 ± 0.02d B 32.57 ± 0.82a AF 14.92 ± 1.52a B
G40 0.19 ± 0.02b A 1.03 ± 0.00d B 20.97 ± 4.41b B 21.42 ± 1.25b D
S30 0.18 ± 0.02c A 1.20 ± 0.06a D 28.07 ± 1.82d BF 7.45 ± 0.56f F
S40 0.19 ± 0.01c A 1.20 ± 0.03a D 31.34 ± 0.51d B 7.29 ± 0.56f C
T30 0.18 ± 0.01d A 1.06 ± 0.19b B 34.19 ± 6.72c AF 18.53 ± 0.75c A
T40 0.26 ± 0.02e B 0.88 ± 0.02f A 18.92 ± 0.60c B 23.61 ± 1.21e D
a

Data (mean ± SD), The letters E, G, S and T indicate to 1-ethyl-3-methylimidazolium acetate, glycerol, sorbitol and triethylene glycol, respectively. The number next to them

b

Different superscript letters in a column indicate that there are statistically significant differences (P < 0.05) between samples. Lower caseletters show statistically analysis for a plasticizer with different weight percentage and capital letters indicate statistically analysis between plasticizers