Table 3.

Effects of plasticizers on mechanical properties of anchote starch films

Films Tensile Strength (MPa) Elongation at Break (%) Modulus of (MPa)

E30 6.18 ± 0.65 49.10 ± 7.76 105.00 ± 32.66
E40 4.19 ± 0.67 42.83 ± 9.44 50.20 ± 13.50
G30 6.45 ± 1.19 34.26 ± 12.42 341 ± 68.00
G40 6.35 ± 0.55 48.95 ± 4.22 133 ± 29.00
S30   -   -   -
S40 15.30 ± 3.91 25.43 ± 8.90 1200 ± 260.00
T30 8.53 ± 1.25 17.40 ± 1.94 727 ± 117.04
T40 7.01 ± 0.57 38.71 ± 5.70 447 ± 29.41
a

Data (mean ± SD), The letters E, G, S and T indicate to 1-ethyl-3-methylimidazolium acetate, glycerol, sorbitol and triethylene glycol, respectively. The number next to them indicates the percentage (w/w) of plasticizer to dry starch ration