Skip to main content
. 2020 Jun 22;78(6):3363–3381. doi: 10.1007/s00289-020-03266-5

Table 2.

Solution and spinning parameters used for the preparation of PC nanofibers with the corresponding fiber average diameter and contact angle values

Sl.no. Concentration of PC solution (w/v%) Solvent ratio Flow rate (mL/h) Working Distance (cm) Voltage (kV) Average diameter (nm) Contact angle (°)
1 14 1:1 0.5 15 20 90 132.8
2 14 3:2 0.5 15 20 388 128.7
3 14 7:3 0.5 15 20 583 119.0
4 14 4:1 0.5 15 20 752 117.7
5 14 9:1 0.5 15 20 816 109.4
6 14 1:1 1.0 15 20 178 121.4
7 14 1:1 1.5 15 20 236 114.3
8 14 1:1 0.5 15 10 137 130.9
9 14 1:1 0.5 15 30 382 124.2
10 14 1:1 0.5 10 20 136 130.4
11 14 1:1 0.5 20 20 238 123.1