Mixture proportions with dosage of raw materials of GO-modified engineered cementitious composite (ECC). (CR—crumb rubber and SP—superplasticizer).

Mix Cement kg/m3 FA kg/m3 Sand kg/m3 CR Water kg/m3 SP kg/m3 PVA GO
% g % kg/m3 % g
1 570 684 451.44 0 0.00 269.61 2.51 2.0 25.08 0.05 9.59
2 570 684 451.44 0 0.00 269.61 2.51 2.0 25.08 0.01 1.92
3 570 684 451.44 0 0.00 269.61 2.51 2.0 25.08 0.03 5.76
4 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.03 5.76
5 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.03 5.76
6 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.03 5.76
7 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.05 9.59
8 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.01 1.92
9 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.03 5.76
10 570 684 451.44 5 759.83 269.61 2.51 2.0 25.08 0.03 5.76
11 570 684 451.44 10 1519.67 269.61 2.51 2.0 25.08 0.05 9.59
12 570 684 451.44 10 1519.67 269.61 2.51 2.0 25.08 0.03 5.76
13 570 684 451.44 10 1519.67 269.61 2.51 2.0 25.08 0.01 1.92