Physicochemical characteristic of the obtained defective TiO2-HIO3_T samples.

Sample BET (m2·g−1) V Pores (cm3·g−1) Eg (ev) Photo
TBT 169 0.0836 3.2 graphic file with name materials-13-02763-i012.jpg
TBT-HIO3_20_300 172 0.0847 2.7 graphic file with name materials-13-02763-i013.jpg
TBT-HIO3_20_400 88 0.0432 2.85 graphic file with name materials-13-02763-i014.jpg
TBT-HIO3_20_450 48 0.0236 2.9 graphic file with name materials-13-02763-i015.jpg
TBT-HIO3_20_650 0.7 0.0003 2.9 graphic file with name materials-13-02763-i016.jpg
TBT-HIO3_20_1000 0.4 0.0002 2.8 graphic file with name materials-13-02763-i017.jpg