Skip to main content
. 2020 May 31;10(6):1079. doi: 10.3390/nano10061079

Table 3.

Modulus of elasticity (E), tensile strength (σuts), and % elongation at break (%ε), of all tested PVOH/ZnO/NaMt nanocomposite films as well as of PVOH/NaMt nanocomposite and pure PVOH film.

Samples Code Names Young’s Modulus-(E) Tensile Strength-(σuts) % Elongation at Break (%ε)
PVOH 2066.6 ± 146.5 6.7 ± 0.5 0.7 ± 0.1
PVOH/NaMt 2602.2 ± 158.8 12.5 ± 0.8 1.2 ± 0.2
PVOH/ZnO/NaMt-4 3154.3 ± 167.3 19.1 ± 0.7 1.0 ± 0.2
PVOH/ZnO/NaMt-2 2546.6 ± 158.5 12.7 ± 0.7 0.8 ± 0.2
PVOH/ZnO/NaMt-1 2328.8 ± 145.2 10.4 ± 0.6 0.8 ± 0.3
PVOH/ZnO/NaMt-0.7 2168.3 ± 163.2 6.3 ± 0.4 0.6 ± 0.1
PVOH/ZnO/NaMt-0.5 1978.2 ± 125.8 5.3 ± 0.4 0.4 ± 0.1
PVOH/ZnO/NaMt-0.4 936.5 ± 98.5 3.1 ± 0.3 0.3 ± 0.1