Comparison of different surface morphologies on plasma-induced crystallization in radio-frequency (RF) oxygen plasma at 800 W plasma power output and different treatment times (1 s and 10 s).

Plasma Treatment
Surface Power (W) Treatment Time (s) Phase
Ti foil - - amorphous
Ti foil 800 1 anatase/rutile
Ti foil 800 10 anatase/rutile
TiO2 NT 15 nm 800 1 anatase
TiO2 NT 15 nm 800 10 rutile
TiO2 NT 100 nm 800 1 anatase
TiO2 NT 100 nm 800 10 anatase/rutile