Table 2.

Melting temperatures, enthalpy and percent crystallinity of specimens with varying AMP percentage. Curve fitting results of different specimens as obtained by power law model (η=kωn-1, Cox−Merz rule); dynamic viscosity was converted into shear viscosity and fitted in the model. k is the flow consistency index and n is the flow behavior index.

Specimen Name Tm ( °C) Hm (J/g) Xcw (%) - DSC k n
0AMP-PEEK 338.21 32.9869 25.38 8400 0.53

5AMP-PEEK 339.10 31.3710 25.67 8900 0.5

10AMP-PEEK 338.91 30.0969 26.31 10500 0.46

15AMP-PEEK 338.20 31.0460 28.76 11600 0.42

R2 > 0.9