Table 4. Direct H2O2 Synthesis and Degradation Testing over Different Catalysts.
| catalyst | H2O2 productiona (mmol gPd–1 h–1) | H2O2 degradationb (mmol kgcat–1 h–1) | H2O2 selectivity (%) |
|---|---|---|---|
| Pd/HTS-1 | |||
| 500 °C, 4 h, air | 5310 | 44,780 | 34.65 |
| +reduced 400 °C, 2 h | 7460 | 70,530 | 18.91 |
| +500 °C, 6 h, air | 2330 | 49,850 | 21.53 |
| Pd@HTS-1 | |||
| 500 °C, 4 h, air | 23,666 | 27,980 | 42.45 |
| +reduced 400 °C, 2 h | 32,370 | 29,880 | 29.78 |
| +500 °C, 6 h, air | 35,705 | 26,650 | 47.69 |
Reaction conditions: H2/Ar (2.9 MPa) and O2/Ar (1.1 MPa), 8.5 g of solvent (2.9 g of HPLC water, 5.6 g of MeOH), 0.02 g of 0.1 wt % Pd catalyst, RT, 1200 rpm, 30 min.
Reaction conditions: H2/Ar (2.9Mpa), 8.5 g of solvent (5.6 g of MeOH, 2.22 g of H2O, and 0.68 g of 30 wt % H2O2), 0.02 g of 0.1 wt % Pd catalyst, RT, 1200 rpm, 30 min.