Skip to main content
. 2020 Jul 18;6(7):e04492. doi: 10.1016/j.heliyon.2020.e04492

Table 5.

Surface characteristics, proximate contents, and elemental analyses of precursor, char, PKSAC and Ag-NPs-PKSAC.

Properties Sample
PKS Char PKSAC Ag-NPs-PKSAC
BET surface area (m2/g) - 248.130 363.423 298.220
Total pore volume (cm3/g) - 0.087 0.169 0.137
Micropore volume (cm3/g) - 0.121 0.146 0.120
Porosity (%) 21 58 62
Average pore diameter (Å) - - - 16.2

Proximate Analysis (%)
Moisture content 7.3 6.6 5.9 5.7
Volatile matter 71.1 29.0 18.9 19.0
Fixed Carbon 18.5 59.7 69.2 69.3
Ash 3.1 4.7 6.0 6.0

Elemental Analysis (%)
Carbon 49.2 63.7 76.3 76.3
Hydrogen 5.9 4.5 4.2 4.2
Nitrogen 0.6 0.5 0.5 0.5
Others 44.3 31.3 19.1 19.0