Table 2. Thermal Properties of PPC and PPC with Networks.
| sample | temperature for onset of weight loss (°C) | temperature for 5% weight loss (°C) | temperature for maximum weight loss (°C) | glass transition temperature (°C) |
|---|---|---|---|---|
| PPC | 197 | 217 | 231/251c | 51,e 35f |
| PPC0.5 | 256,a 256b | 288,a 277b | 298,a 293b | 47, 31 |
| PPC1 | 264, 258 | 288, 281 | 297, 294 | 50, 33 |
| PPC2 | 273, 264 | 289, 282 | 297, 293 | 50, 34 |
| PPC3 | 272, 263 | 292, 282 | 302, 295 | 53, 38 |
| PPC4 | 275, 266 | 291, 282 | 312, 288/299d | 51, 37 |
The copolymers.
The soluble fraction of the copolymers.
PPC has two main maximum weight-loss peaks at 231 and 251 °C.
The soluble fraction of the PPC4 has two maximum weight-loss peaks at 288 and 299 °C.
Measured from tan δ curves in a DMA test.
Measured from DSC curves.