Skip to main content
. 2020 Jul 9;23(8):101353. doi: 10.1016/j.isci.2020.101353

Table 2.

WVTRs for Polymer Films with 25 nm ALD Al2O3Deposited at 100°C(Vähä-Nissi et al., 2015)

Oxidizing Precursor WVTR (23°C, 50% RH) g/m2/day
A-CEL 290
A-CEL + ALD <1.0
CEL 100
CEL + ALD 44
C-CEL 35
C-CEL + ALD 2
BOPP <1.0
BOPP + ALD <1.0
PHB/HV 8.3
PHB/HV + ALD 1.0
O-PA <1.0
O-PA + ALD <1.0
O-PET 3.1
O-PET + ALD <1.0
PLA 21
PLA + ALD <1.0

A-CEL, anchored cellulose; CEL, cellulose; BOPP, biaxially oriented polypropylene; O-PA, oriented polyamide and polyethylene; O-PET, oriented polyethylene terephthalate.