Skip to main content
. 2020 Jun 27;12(7):1440. doi: 10.3390/polym12071440

Table 3.

Thermal properties on cooling and second heating differential scanning calorimetry (DSC) scans of the samples.

Processing Cycle Number Sample Cooling Second Heating
Tc * (°C) Tm * (°C) ΔHm (J/g) Χc (%)
1 PP 114 166 91 44
PP-Bag. 122 163 75 45
PP-Bag. +alk. 121 165 74 44
PP-Bag. +alk. +sil. 118 166 99 59
3 PP 116 165 101 49
PP-Bag. 119 165 80 49
PP-Bag. +alk. 121 163 84 50
PP-Bag. +alk. +sil. 122 165 100 60
5 PP 114 166 95 46
PP-Bag. 121 164 75 46
PP-Bag. +alk. 121 164 78 47
PP-Bag. +alk. +sil. 121 162 83 50

* Tc and Tm were taken at the maximum peak of crystallization and melting peaks.