. 2020 Jun 27;12(7):1440. doi: 10.3390/polym12071440

Table 4.

Thermal degradation data of PP and PP-Bagasse biocomposites.

Processing Cycle Sample Degradation Stage TO (°C) Tmax (°C)
First cycle PP 1 408 455
PP-Bag. 1 271 354
2 423 462
PP-Bag. +alk. 1 314 363
2 438 461
PP-Bag. +alk. +sil. 1 317 360
2 447 468
Third cycle PP 1 373 445
PP-Bag. 1 271 363
2 431 463
PP-Bag. +alk. 1 309 358
2 431 468
PP-Bag. +alk. +sil. 1 310 358
2 428 457
Fifth cycle PP 1 371 431
PP-Bag. 1 287 366
2 430 472
PP-Bag. +alk. 1 318 360
2 417 440
PP-Bag. +alk. +sil. 1 322 360
2 434 461