Skip to main content
. 2020 Jun 27;12(7):1440. doi: 10.3390/polym12071440

Table 5.

Dynamic mechanical analysis (DMA) results of the studied materials.

Processing Cycle Number Sample Tg (°C) * E′ (MPa) at 25 °C Full Width at Half Maximum (FWHM) of Tan δ Peaks Tan δ Peaks Height
1 PP 7.9 1481 24.4 0.091
PP-Bag. 8.2 1741 23.3 0.083
PP-Bag. +alk. 8.1 2261 21.9 0.081
PP-Bag. +alk. +sil. 8.6 1962 22.2 0.081
3 PP 8.4 1453 24.9 0.087
PP-Bag. 8.3 1810 22.5 0.087
PP-Bag. +alk. 7.3 2319 20.7 0.078
PP-Bag. +alk. +sil. 7.9 1835 20.5 0.080
5 PP 7.0 1383 23.4 0.093
PP-Bag. 8.9 1905 22.7 0.083
PP-Bag. +alk. 8.1 2111 21.1 0.080
PP-Bag. +alk. +sil. 8.2 1899 21.8 0.078

* Tg values of the PP phase were taken at the maximum peak of the tan delta curves.