Parts Tm (°C) Hm (J/g) χc (%)
PA610 224.2 ± 1.5 62.9 ± 0.9 31.9 ± 0.8
PA610/10HNTs 225.4 ± 1.1 43.4 ± 1.1 24.5 ± 0.9
PA610/20HNTs 225.6 ± 0.9 40.3 ± 1.2 25.6 ± 1.0
PA610/30HNTs 225.8 ± 0.8 34.6 ± 0.9 25.1 ± 0.8