Table 4.
Polyol Used for the Ester Foam. | Reference | EXP. 1 | EXP. 2 | EXP. 3 |
---|---|---|---|---|
Desmophen 2200B (virgin polyol) (%) | 100.0 | 99.0 | 99.0 | 99.0 |
Recycled polyol (%) | 0.0 | 1.0 | 1.0 | 1.0 |
Foam Physical Properties | ||||
Rise time (s) | 119.0 | 117.0 | 118.0 | 117.0 |
Foam settling (%) | 1.20 | 2.10 | 2.00 | 1.50 |
Density (kg/m3) | 25.10 | 24.46 | 24.48 | 24.25 |
Hardness CFD-40% (kPa) | 4.80 | 4.42 | 4.46 | 4.24 |
Compression set 22 h 75% 70 °C (%) | 8.00 | 9.85 | 9.70 | 10.05 |
Airflow (L/min) | 33.0 | 21.0 | 25.0 | 25.0 |
Tensile strength (kPa) | 107.0 | 144.0 | 124.0 | 132.0 |
Cell structure (fine 1.... coarse 8) | 5.0 | 4.0 | 4.0 | 4.0 |