. 2020 Jul 10;12(7):1533. doi: 10.3390/polym12071533

Table 4.

Properties of the foams obtained using the ester formulation presented in Table 1, replacing 1 pbw virgin polyol (Desmophen 2200B) with recycled polyol. CFD: compression force deflection.

Polyol Used for the Ester Foam. Reference EXP. 1 EXP. 2 EXP. 3
Desmophen 2200B (virgin polyol) (%) 100.0 99.0 99.0 99.0
Recycled polyol (%) 0.0 1.0 1.0 1.0
Foam Physical Properties
Rise time (s) 119.0 117.0 118.0 117.0
Foam settling (%) 1.20 2.10 2.00 1.50
Density (kg/m3) 25.10 24.46 24.48 24.25
Hardness CFD-40% (kPa) 4.80 4.42 4.46 4.24
Compression set 22 h 75% 70 °C (%) 8.00 9.85 9.70 10.05
Airflow (L/min) 33.0 21.0 25.0 25.0
Tensile strength (kPa) 107.0 144.0 124.0 132.0
Cell structure (fine 1.... coarse 8) 5.0 4.0 4.0 4.0