Parameters of the instantaneous corrosion process for the samples studied in Black Sea water.

Sample C45 I-Zn II-Zn/Fe III-Mn OPS PPS
E(I = 0), mV −636 −748 −578 −766 −581 −163
Rp, kΩ·cm2 1.83 2.74 2.04 0.644 4.11 0.715
jcor, µA/cm2 18.41 15.94 15.97 51.26 9.38 57.91
vcor, µm/year 223.9 193.8 194.1 623.5 114.0 704.4
ba, mV/decade 193 393 110 217 223 248
bc, mV/decade −210 −211 −279 −184 −275 −551