Skip to main content
. 2020 Aug 25;15:6433–6449. doi: 10.2147/IJN.S261483

Table 2.

Mechanical Properties of Electrospun CET’s Protein–CS–PEO Nanofibers Before and After GA Vapor and HT Crosslinking

Sample Ultimate Tensile Strength (MPa) Ultimate Strain (%) Young’s Modulus (MPa)
Non-crosslinked
 C1 1.72 ± 0.09 55.55 ± 10.47 10.19 ± 0.71
 C2 1.30 ± 0.08 29.62 ± 8.63 22.60 ± 4.33
 C3 1.29 ± 0.14 12.02 ± 1.0 14.85 ± 1.16
 C4 1.27 ± 0.16 6.39 ± 3.31 35.70 ± 3.33
GA vapor crosslinked
 C1 5.04 ± 0.09 3.88 ± 0.45 139.94 ± 8.77
 C2 2.94 ± 0.57 2.17 ± 0.29 147.57 ± 11.91
 C3 5.70 ± 0.06 10.92 ± 0.19 148.12 ± 8.65
 C4 4.88 ± 0.14 2.07 ± 0.14 279.61 ± 10.58
HT crosslinked
 C3 4.81 ± 0.22 6.69 ± 0.85 90.94 ± 5.78
 C4 4.49 ± 0.14 6.42 ± 0.79 94.91 ± 5.30

Abbreviations: GA vapor crosslinked, glutaraldehyde vapor crosslinked; HT crosslinked, heat treatment crosslinked.