Skip to main content
. 2020 Jul 22;12(8):1627. doi: 10.3390/polym12081627

Table 4.

Tpeak of PP, wood and PP-based WPCs.

Sample Heating Rate (°C/min) Atmosphere Tpeak (°C)
Hemicellulose Cellulose Lignin PP
Wood 5 °C/min N2 290.3 335.96 NA -
Air 267.9 308.5 442.2 -
PPVW00 N2 - - - 430.5
Air - - - 331.7
PPVW40 N2 291.2 342.8 NA 435.7
Air 288.3 337.4 456.4 364.0
PPVW60 N2 291.4 344.5 NA 439.6
Air 290.1 336.7 453.9 364.5
Wood 10 °C/min N2 293.3 347.5 NA -
Air 280.0 321.0 464.1 -
PPVW00 N2 - - - 440.1
Air - - - 351.1
PPVW40 N2 295.1 349.6 NA 441.9
Air 288.9 347.2 471.1 380.3
PPVW60 N2 296.3 351.8 NA 449.6
Air 288.7 342.4 468.4 374.4
Wood 20 °C/min N2 311.5 359.5 NA -
Air 292.5 335.7 482.2 -
PPVW00 N2 - - - 460.0
Air - - - 394.2
PPVW40 N2 317.6 368.0 NA 464.8
Air 308.4 358.2 496.1 393.4
PPVW60 N2 319.5 370.5 NA 468.6
Air 309.3 356.5 475.4 394.1
Wood 40 °C/min N2 322.4 372.1 NA -
Air 305.2 350.2 501.1 -
PPVW00 N2 - - - 479.0
Air - - - 430.1
PPVW40 N2 331.0 380.1 NA 485.2
Air 311.0 370.4 536.4 425.7
PPVW60 N2 334.8 384.0 NA 486.1
Air 310.8 369.3 535.7 422.5