Compounding procedure for the styrene butadiene rubber (SBR) binary filler compounds.

Stage 1
0–20″ Rubbers (initial temperature: 110 °C)
20″–1′00 1/2 filler (carbon black)
1′00″–1′40″ 1/2 filler (carbon black)
1′40″–2′40″ Oil
2′40″–3′40″ 1/2 filler (silica), 1/2 silane
3′40″–4′40″ 1/2 filler (silica), 1/2 silane
4′40″–5′40″ ZnO, Stearic acid, 6PPD, TMQ
5′40″–10′40″ Extra mix and dump (dump temperature: 150–155 °C)
Stage 2
0–20″ Compounds of stage 1 (initial temperature: 50 °C)
20″–1′ Sulfur, cure accelerators (TBBS, DPG, PVI)
1′–2′ Extra mix and dump (dump temperature: 100 °C))