Thermal properties of PLA composites for a heating rate of 10 °C/min.

Sample Tg1,2 (°C) Tcc (°C) ΔHcc (J/g) Tm (°C) ΔHm (J/g) Xcc (%)
Neat PLA 59.6 126.2 39.6 166.1 41.0 44.1
PL7/3 −47.5, 60.3 137.9 9.0 167.0 9.5 10.2
PLM1 −46.5, 60.3 138.7 3.1 167.0 3.2 3.5
PLM3 −46.1, 60.7 139.7 2.6 167.4 2.6 2.8
PLM5 −47.8, 61.1 141.7 1.8 167.6 1.8 2.0
PLM7 −47.6, 61.4 142.5 1.7 167.4 1.7 1.9
PLMS1 −47.4, 60.6 138.3 13.2 167.2 13.3 14.3
PLMS3 −46.2, 61.4 140.6 11.3 168.3 11.5 12.3
PLMS5 −46.8, 61.6 138.2 16.7 167.1 16.8 18.1
PLMS7 −47.7, 61.8 136.3 21.8 167.1 21.9 23.5