Table 3.
Yield strength, toughness and Young's modulus of pure PS film, ANMs-C3H5-X/PS, and ANMs-C7H8-X/PS composite films.
| Sample notation | Yield strength (MPa) | Toughness (N/mm2) | Young's modulus (MPa) |
|---|---|---|---|
| Pure PS | 12.93 | 0.08 | 1,514.00 |
| ANMs-C3H5-50% | 24.78 (91.65%) | 0.73 (812.50%) | 1,653.66 (9.22%) |
| ANMs-C3H5-100% | 21.78 (68.45%) | 0.50 (525.00%) | 1,827.09 (20.68%) |
| ANMs-C3H5-200% | 20.49 (58.47%) | 0.42 (425.00%) | 1,685.88 (11.35%) |
| ANMs-C7H8-50% | 14.39 (11.29%) | 0.49 (521.50%) | 1,117.97 (−26.16%) |
| ANMs-C7H8-100% | 21.59 (66.98%) | 0.28 (250.00%) | 2,069.26 (36.68%) |
| ANMs-C7H8-200% | 21.97 (69.45%) | 0.29 (262.50%) | 1,913.88 (26.41%) |