Skip to main content
. 2020 Jun 18;11(27):7102–7122. doi: 10.1039/d0sc02589e

Table 1. Elemental compositions, micropore volumes, and H+ densities of H-Al-Beta-F and their dealuminated analogs.

Sample Si/Al a V micro b /cm3 g–1 H+/Al (NH4+) c H+/Al (DTBP) d H+ c /u.c. V micro b (de-Al) e
Si-Beta-F 0.21 0
H-Al-Beta-F(2.0) 23 0.22 0.75 0.54 2.0 0.22
H-Al-Beta-F(1.4) 34 0.18 0.78 1.4 0.21
H-Al-Beta-F(1.2) 45 0.20 0.84 0.79 1.2 0.21
H-Al-Beta-F(0.78) 65 0.21 0.79 0.78 0.20
H-Al-Beta-F(0.57) 93 0.23 0.84 0.57 0.22
H-Al-Beta-F(0.16) 220 0.20 0.54 1.1 0.16
H-Al-Beta-F(0.11) 500 0.20 0.84 0.11
H-Al-Beta-OH(1.7) 40 0.23 1.1 0.38 1.7

aDetermined by AAS.

bDetermined by minimum in ∂Vads/∂ log(P/P0) in N2 adsorption isotherms.

cDetermined by TPD of NH3 after aqueous-phase ion exchange with 1 M NH4NO3, 24 h, 353 K.

dDetermined by in situ 2,6-di-tert-butylpyridine titration during ethanol dehydration catalysis (378 K, 5 kPa C2H5OH, 1 kPa H2O).

e“de-Al” reflects deAl-Beta samples generated by treatment of H-Al-Beta in 69% HNO3 (353 K, 16 h).