Weibull strength (σ0) and Weibull modulus (m) data for the four types of 3D printed resin specimens according to post-curing time.

Specimen Post-Curing Time m σ0, MPa
Nextdent C&B Control 6.71 (6.23–7.19) 106.37
15 min 7.42 (6.01–8.82) 107.40
30 min 6.21 (5.35–7.07) 111.79
60 min 9.82 (8.35–11.29) 103.39
90 min 9.49 (7.53–11.45) 127.52
120 min 10.95 (9.43–12.47) 135.58
Nextdent C&B MFH Control 11.46 (9.89–13.02) 127.17
15 min 10.69 (9.25–12.12) 123.32
30 min 11.05 (9.17–12.93) 132.18
60 min 9.20 (8.17–10.23) 152.83
90 min 14.24 (11.41–17.07) 152.11
120 min 16.43 (13.80–19.06) 154.87
ZMD-1000B temporary Control 7.87 (5.81–9.92) 121.26
15 min 8.88 (7.51–10.25) 117.95
30 min 12.25 (10.24–14.25) 120.03
60 min 13.54 (11.18–15.90) 127.37
90 min 14.91 (13.23–16.59) 139.44
120 min 18.09 (14.17–22.00) 145.81
DIOnavi C&B Control 5.30 (4.57–6.03) 125.00
15 min 11.48 (9.67–13.30) 124.25
30 min 12.42 (9.18–15.66) 127.67
60 min 11.35 (9.61–13.09) 122.91
90 min 17.84 (15.87–19.8) 138.14
120 min 16.44 (14.43–18.46) 143.18