Skip to main content
. 2020 Dec 7;13(23):5576. doi: 10.3390/ma13235576

Table 3.

Mix proportions of alkali-activated coal gangue-slag concrete (kg/m3).

Specimens Cementitious Materials Water Na2SiO3
Solution
NaOH
Solution
Aggregates Compressive Strength/MPa
Coal Gangue Slag Sand Coal Gangue Gravel 28 d 90 d
OPC - - 200 - - 565 - 1050 46.1 53.2
W0 280 280 138.24 172.83 28.02 565 0 1050 62.1 66.8
W30 280 280 138.24 172.83 28.02 565 315 735 54.2 56.3
W50 280 280 138.24 172.83 28.02 565 525 525 53.2 53.4
W70 280 280 138.24 172.83 28.02 565 735 315 48.7 48.3
W100 280 280 138.24 172.83 28.02 565 1050 0 42.7 40.5
S30 280 280 138.24 172.83 28.02 565 315 735 58.4 59.3
S50 280 280 138.24 172.83 28.02 565 525 525 57.7 57.9
S70 280 280 138.24 172.83 28.02 565 735 315 55.1 55.2
S100 280 280 138.24 172.83 28.02 565 1050 0 49.3 48.7

W stands for uncalcined, S stands for calcined.