表 5.
光照强度及时间对双重固化树脂水门汀氧阻聚层厚度的影响
Effect of light intensity and illumination time on oxygen inhibition layer thickness of dual-cured resin cement /μm
| Items | 10 s | 20 s | 40 s | 60 s | F | P |
| n=5 | ||||||
| 800 mW/cm2 | 26.40±2.19 | 24.80±1.79 | 23.2±1.79 | 19.2±3.35 | 8.524 | < 0.001 |
| 1 000 mW/cm2 | 20.80±1.79 | 19.20±5.22 | 20.00±2.83 | 19.20±3.35 | 0.237 | 0.870 |
| 1 200 mW/cm2 | 20.00±2.83 | 17.60±2.19 | 17.60±2.19 | 17.60±2.19 | 0.471 | 0.636 |
| F | 11.400 | 6.091 | 7.400 | 1.286 | ||
| P | 0.002 | 0.015 | 0.008 | 0.313 | ||