Table 6.

Aging effect of PEDOT:PSS coated conductive yarns.

Conductive Yarn Type Aging Duration (Week) Electrical Resistance (KΩ)
For 1st Coating For 2nd Coating
Mean SD Increased Electrical Resistance Every Week (%) Total Increased Electrical Resistance (%) from Week 0–Week 5 (%) Mean SD Increased Electrical Resistance (%) Total Increased Electrical Resistance (%) from Week 0–Week 5 (%)
PP 0 131.00 3.41 - 23.43 43.00 2.08 - 20.98
1 143.07 1.63 9.21 44.70 0.46 3.95
2 149.67 0.57 4.61 46.93 0.57 4.99
3 154.70 2.03 3.36 48.73 0.75 3.84
4 159.30 1.91 2.97 51.37 1.32 5.42
5 164.53 0.83 3.28 52.80 0.30 2.78
PLA 0 223.00 7.76 - 26.85 122.00 5.47 - 23.00
1 251.10 1.11 12.60 134.13 1.05 9.94
2 262.40 2.80 4.50 139.40 1.20 3.92
3 269.10 1.74 2.55 143.33 0.86 2.82
4 279.10 2.16 3.72 148.50 0.86 3.61
5 288.80 2.35 3.48 152.53 0.83 2.71
PP/PLA 0 181.00 3.63 - 25.45 66.00 1.23 - 21.96
1 199.50 0.79 10.22 73.43 0.65 11.26
2 210.50 1.12 5.51 75.67 0.57 3.05
3 215.33 0.96 2.29 78.50 0.87 3.74
4 223.40 0.79 3.75 80.80 0.36 2.93
5 231.63 0.42 3.68 81.63 0.87 1.03