Table 4.

The average values of the LDPE plate microhardness (HIT—indentation hardness; HV—Vickers microhardness; and hm—maximum impression depth). Standard deviations are provided in parentheses.

Samples HIT HV hm
(MPa) (-) (µm)
LDPE 20.9 (1.6) 2.0 (0.2) 37.4 (1.8)
LDPE_1% ZnO/V 27.1 (0.5) 2.6 (0.1) 31.8 (0.2)
LDPE_3% ZnO/V 26.6 (0.7) 2.5 (0.1) 32.0 (0.3)
LDPE_5% ZnO/V 25.3 (1.3) 2.4 (0.1) 32.9 (0.7)
LDPE_1% ZnO/V_CH 27.2 (0.6) 2.6 (0.1) 31.7 (0.3)
LDPE_3% ZnO/V_CH 16.7 (1.4) 1.6 (0.1) 41.9 (1.7)
LDPE_5% ZnO/V_CH 23.0 (1.3) 2.2 (0.1) 34.8 (0.9)