Mechanical properties for CMCas films synthesized with various NaOH concentrations.

Type of Film Tensile Strength (MPa) Elongation at Break (%)
20 g/100 mL NaOH-CMCas 36.30 ± 1.32 c 13.00 ± 7.22 c
30 g/100 mL NaOH-CMCas 41.78 ± 3.28 b 24.99 ± 3.79 a
40 g/100 mL NaOH-CMCas 44.59 ± 1.73 a 17.32 ± 4.21 b
50 g/100 mL NaOH-CMCas 28.97 ± 2.06 d 9.52 ± 2.57 c
60 g/100 mL NaOH-CMCas 27.55 ± 1.72 d 2.38 ± 0.88 d

Mean ± Standard deviation values within a column in the same group, followed by the different letters (a–d) are significantly different (p < 0.05).