Summary of the mass of polymers and volume of solvents used for 80/20 blend ratio for various blend families.

blend family solution A solution B
polyhydroxybutyrate (PHB)/kappa-carrageenan (KCG) 400 mg of PHB in 8 ml of HFIP 100 mg of KCG in 2 ml of CHCl3
poly(hydroxybutyrate-co-valerate) (PHBV)/KCG 1200 mg of PHBV in 8 ml of HFIP 300 mg of KCG in 2 ml of CHCl3
polydioxanone (PDX)/fucoidan (FUC) 1400 mg of PDX in 9 ml of HFIP 350 mg of FUC in 1 ml of DMF
PDX/KCG 1200 mg of PDX in 7 ml of HFIP 300 mg of KCG in 3 ml of CHCl3
PDX/PHBV 800 mg of PDX and 200 mg of PHBV were dissolved in 10 ml of HFIP
PDX/polysucrose (PSuc) 960 mg of PDX and 240 mg of PSuc were dissolved in 10 ml of HFIP
poly-l-lactic acid (PLLA)/PSuc 800 mg of PLLA and 200 mg of PSuc were dissolved in 10 ml of HFIP
PLLA/cellulose acetate (CA) 800 mg of PLLA in 8 ml of HFIP 200 mg of CA in 2 ml of HFIP
PDX/CA 800 mg of PDX in 6.7 ml of HFIP 200 mg of CA in 1.7 ml of HFIP
PLLA/CA 1% nanosilica to a 80/20 solution of PLLA/cellulose acetate, 1% nanosilica (10 mg) was added and allowed to stir overnight
PDX/CA 1% nanosilica to a 80/20 solution of PDX/cellulose acetate, 1% nanosilica (10 mg) was added and allowed to stir overnight