Thermophysical characteristics of PLA/NR nonwoven fiber samples: initially and after 180 days of water degradation.

NR, wt.% Initial Samples After Water Influence for 180 Days
Tg, °C
(Δ ± 0.5 °C)
Tm, °C
(Δ ± 0.5 °C)
χcr, %
(Δ ± 1%)
Tg, °C
(Δ ± 0.5 °C)
Tm, °C
(Δ ± 0.5 °C)
χcr, %
(Δ ± 1%)
0 61 164 34 -- 168 46
5 63 168 36 -- 167 46
10 66 167 38 -- 167 47
15 65 166 37 -- 166 47