Microhardness and tensile properties of Co29Cr6Mo-xCu alloys [20].

Alloys Microhardness (HV) Tensile strength (MPa)
Elongation (%)
0.2% YS UTS
Co29Cr6Mo–0Cu 298.33 ± 29.41 423.61 ± 18.21 576.92 ± 50.36 10.7 ± 1.8
Co29Cr6Mo–1Cu 292.69 ± 28.63 310.38 ± 41.43 447.83 ± 24.85 18.5 ± 3.7
Co29Cr6Mo–2Cu 279.67 ± 26.79 432.73 ± 12.86 499.13 ± 21.65 11.5 ± 3.8
Co29Cr6Mo–4Cu 274.64 ± 26.05 440.53 ± 36.47 620.56 ± 15.24 15.2 ± 0.1