Skip to main content
. 2021 Feb 5;7(2):e06176. doi: 10.1016/j.heliyon.2021.e06176

Table 4.

Mean values and standard deviation of parameters obtained by DSC (glass transition temperature of PLA) and TGA (Maximum degradation temperature (TPeak) and Initial degradation temperature (T0)) of studied films conditioned at 53 % R.H. and 25 °C.

Formulations DSC
TGA
Tg (°C) TPeak (°C) T0 (°C)
PLA 54.24 ± 0.3b 315.6 ± 0.5a 245.0 ± 0.2b
TPS --- 337.5 ± 1.1c 236.1 ± 0.5a
PLA75/TPS25 50.6 ± 0.5a 342.4 ± 0.9d 267.33 ± 0.5c
PLA75/TPS25/ESO1.5 57.2 ± 1.6c 341.3 ± 0.5d 265.95 ± 0.3c
PLA75/TPS25/ESO3 57.9 ± 1.3c 329.7 ± 0.5b 285.13 ± 0.5d

Different superscript letters mean significant differences (p < 0.05) between formulations.