Surface treatment Aging Ra (μm) Biaxial strength (MPa) Monoclinic phase (vol%)
As Sintered Baseline 0.32 (0.10) 908 (131) < 1
Autoclave 0.33 (0.15) 724 (188) ~8
Thermocycling 0.31 (0.10) 689 (185) ~11
Grind Baseline 0.87 (0.16) 1298 (194) ~32
Autoclave 1.32 (0.30) 1009 (147) ~33
Thermocycling 1.00 (0.19) 926 (182) ~31
Grind + Polish Baseline 0.55 (0.12) 1224 (149) ~28
Autoclave 0.43 (0.12) 1085 (77) ~27
Thermocycling 0.55 (0.15) 1086(144) ~28