Skip to main content
. 2021 Feb 25;13(5):696. doi: 10.3390/polym13050696

Table 1.

Tensile strength, elongation at break, and tearing strength of PLA and Chitosan–PLA films.

Composition Tensile Strength
(kgf/cm2)
Elongation at Break
(%)
Tearing Strength
(gf)
MD TD MD TD MD TD
PLA 448 ± 19 a 271 ± 18 a 318 ± 16 b 498 ± 41 a 54 ± 7 c 220 ± 14 c
0.5% CH–PLA 261 ± 23 b 139 ± 8 b 376 ± 37 a 416 ± 39 a 81 ± 7 b 282 ± 14 a
1% CH–PLA 216 ± 3 c 133 ± 12 b 320 ± 7 b 414 ± 67 a 97 ± 12 a 252 ± 13 b
2% CH–PLA 155 ± 8 d 79 ± 6 c 255 ± 11 c 271 ± 32 b 84 ±8 b 226 ± 24c

MD, machine direction; TD, transverse direction; 0.5% CH–PLA, 1% CH–PLA, and 2% CH–PLA, PLA containing 0.5%, 1%, and 2% chitosan, respectively. Data are presented as mean ± SD (n = 3). Different superscript in the same column indicates significant difference (p < 0.05).