Table 5. Parameters from Tensile Tests for the TPWF-Based Films.
Young’s modulus, E (MPa) | maximum stress, σmax (MPa) | strain at maximum stress, εmax σ (%) | stress at break, σb (MPa) | strain at break, εb (%) | |
---|---|---|---|---|---|
TPWF | 4.7 ± 0.1 | 0.6 ± 0.1 | 45.8 ± 4.9 | 0.32 ± 0.1 | 48.4 ± 4.7 |
PBS | 402 ± 23 | 22.7 ± 1.6 | 10.8 ± 2.8 | 22.6 ± 1.6 | 10.8 ± 2.8 |
Co | 120 ± 5 | 18.4 ± 1.4 | 240 ± 36 | 12.2 ± 3.5 | 253 ± 34 |
70TPWF/30PBS | 83.2 ± 7.6 | 3.6 ± 0.1 | 8.8 ± 1.5 | 3.5 ± 01 | 8.9 ± 1.7 |
70TPWF/25PBS/5Co | 72.0 ± 7.3 | 2.9 ± 0.4 | 8.1 ± 0.6 | 2.8 ± 0.4 | 8.2 ± 0.6 |
70TPWF/20PBS/10Co | 69.9 ± 8.6 | 2.7 ± 0.4 | 7.5 ± 0.5 | 2.6 ± 0.3 | 7.6 ± 0.5 |
70TPWF/15PBS/15Co | 62.2 ± 3.0 | 2.8 ± 0.1 | 11.0 ± 0.1 | 2.6 ± 0.2 | 11.1 ± 0.1 |
70TPWF/10PBS/20Co | 56.2 ± 3.9 | 3.1 ± 0.2 | 12.9 ± 1.2 | 3.0 ± 0.3 | 13.0 ± 1.3 |
70TPWF/5PBS/25Co | 37.4 ± 2.6 | 2.7 ± 0.2 | 20.5 ± 1.1 | 2.52 ± 0.2 | 21.0 ± 1.1 |