Skip to main content
. 2021 Apr 15;13(8):1288. doi: 10.3390/polym13081288

Table 1.

Chromaticity coordinates, color variation, and opacity index of developed films.

Films Thickness (µm) L* a* b* ΔE* Opacity
PLA 79.4 ± 6.9 a 98.2 ± 0.1 d −0.05 ± 0.01 f 2.2 ± 0.1 a 0.6 ± 0.1 a
B 81.3 ± 6.8 a 97.5 ± 0.1 b −0.09 ± 0.01 e 2.4 ± 0.1 c 0.8 ± 0.1 b 12.8 ± 1.3 d
B-Q 83.6 ± 8.9 a 97.1 ± 0.1 a −0.51 ± 0.03 c 3.4 ± 0.1 e 1.7 ± 0.1 d 7.4 ± 2.1 c
B-Q-CNC 83.5 ± 8.1 a 97.2 ± 0.1 a −0.44 ± 0.02 d 3.2 ± 0.1 d 1.5 ± 0.1 c 7.2 ± 1.9 c
T 99.0 ± 3.5 a 98.3 ± 0.1 d −0.11 ± 0.01 e 2.3 ± 0.1 b 0.2 ± 0.1 a 3.7 ± 0.3 b
T-Q 102.2 ± 5.2 b 97.9 ± 0.1 c −0.57 ± 0.02 b 3.9 ± 0.1 f 1.9 ± 0.1 e 3.6 ± 0.6 b
T-Q-CNC 103.7 ± 4.3 b 97.9 ± 0.1 c −0.61 ± 0.02 a 3.9 ± 0.1 f 1.9 ± 0.1 e 3.1 ± 0.2 b

Lower case letters a–findicate statistically significant differences of the same parameter among films according to ANOVA analysis (p < 0.05).