Table 4.

Fast pyrolysis of different plastic wastes.

Plastic Type, Temp., Ref. Liquid/Wax Yield (wt.%) Solid Residues Yield (wt.%) Gas Yield (wt.%) Gasoline (C6–C12)
(wt.%)
Diesel (C13–C20)
(wt.%)
Wax (C20+)
(wt.%)
Monomer Recovery (wt.%)
PP-668 °C-[52] 43 2 54 40 - - 26
PP-703 °C-[52] 35 6 57 34 - - 27
PP-746 °C-[52] 29 4 65 29 - - 17
PE-728 °C-[52] 38 2 59 36 - - 34
HDPE-600 °C-[53] 95 - 5 18 25 53 4
HDPE-650 °C-[53] 85 - 15 27 21 37 12
HDPE-700 °C-[53] 60 - 40 32 17 11 37
HDPE-428 °C-[53] 93 - 7 52 33 17 -
PP-409 °C-[53] 96 - 4 70 21 9 -
HDPE-650 °C-[54] 80 - 20 10 18 52 -
PVC-740 °C-[55] 28 49 15 - - - -