Table 5.

Physical-mechanical properties of CDET/NMM and chrome tanned leather.

Test CDET/NMM (a) Chrome (b)
Tensile strength (N/mm2) (c,d) 20.0 ± 0.5 25.0 ± 0.8
Tear strength (N/mm) (c,e) 36.5 ± 0.3 40.0 ± 0.5
Elongation (%) (c,d) 44.5 ± 1.0 46.0 ± 0.8
Resistance to grain cracking (N/mm2) (c,f) 9.3 ± 0.2 10.0 ± 0.1

(a) Crust leather samples prepared by tanning with 3.1/1.9 wt/wt CDET/NMM by weight of the hide processed and retanning with synthetic tannins (see experimental section). (b) Crust leather samples prepared by tanning with 5 %wt basic chromium sulfate and retanning with synthetic tannins. (c) Average of mean and cross backbone samples. (d) Measured according to EN ISO 3376 (IULTCS/IUP 6, 2011). (e) Measured according to EN ISO 3377-1 (IULTCS/IUP 40, 2011). (f) Measured according to EN ISO 3378 (IULTCS/IUP 12, 2002).