Table 7.
Sample | Thickness (mm) | TS (MPa) | EAB (%) | |
---|---|---|---|---|
composite C | thin | 0.095± 0.008 d | 21.22 ± 4.34 a | 37.75 ± 6.12 c |
nanocomposite I | 0.102 ± 0.005 c | 20.98 ± 1.97 a | 60.14 ± 5.27 ab | |
nanocomposite II | 0.107 ± 0.008 c | 20.49 ± 3.22 a | 59.23 ± 8.01 ab | |
composite C | thick | 0.205 ± 0.012 b | 8.43 ± 1.79 b | 52.50 ± 6.37 b |
nanocomposite I | 0.216 ± 0.024 a | 8.15 ± 1.32 b | 66.52 ± 9.98 a | |
nanocomposite II | 0.219 ± 0.009 a | 8.10 ± 1.85 b | 64.29 ± 8.04 a |
TS—Tensile strength, E—Elongation at break. Parameters in columns denoted with the same letters (a. b. c. etc.) do not differ statistically at the level of confidence 0.05.